HASTELLOY® alloy C-276b

Request a quote

Average Tensile Data

Form

Condition

Test Temp °F (°C)

UTS Ksi

YS
0.2%  Ksi

Elon. in 2"
(%)

Sheet, 0.078" (2.0mm) thick

Heat-Treated
at 2050 °F (1121 °C)
Rapid Quenched

Room
400 (204)
600 (316)
800 (427)

114.9
100.6
98.8
94.3

51.6
42.0
35.9
32.7

61
59
68
67

Sheet, 0.094" (2.4mm) thick

Heat-Treated
at 2050 °F (1121 °C)
Rapid Quenched

400 (204)
600 (316)
800 (427)

101.0
97.6
93.5

39.9
33.5
29.7

58
64
64

Sheet 0.063 to 0.187" (1.6 to 4.7mm) thick

Heat-Treated
at 2050 °F (1121 °C)
Rapid Quenched

400 (204)
600 (316)
800 (427)
1000(538)

100.8
97.0
95.0
88.9

42.1
37.7
34.8
33.8

56
64
65
60

Plate 3/16 to 1" (4.8 to 25.4mm) thick

Heat-Treated
at 2050 °F (1121 °C)
Rapid Quenched

400 (204)
600 (316)
800 (427)
1000(538)

98.9
94.3
91.5
87.2

38.2
34.1
32.7
32.8

61
66
60
59

Plate 1" (25.4mm) thick

Heat-Treated
at 2050 °F (1121 °C)
Rapid Quenched

Room
600 (316)
800 (427)

113.9
96.3
94.8

52.9
36.2
30.5

59
63
61